Sifat mekanik:

Standar

sasmita

Kekuatan tarik (MPa)

Kekuatan hasil (MPa)

Elongation (%)

EN10216-1

P195

320440

≥195

≥27

P235

360500

≥235

≥25

P265

410570

≥265

≥23

EN10216-2

P195GH

320440

≥195

≥27

P235GH

360500

≥235

≥25

P265GH

410570

≥265

≥23

13CrMo4-5

440590

≥290

≥22

10CrMo9-10

480630

≥280

≥22

Komposisi kimia:

Standar

sasmita

Komposisi kimia

C

Si

Mn

P

S

Cr

Mo

Cu

Ni

V

EN10216-1

P195

≤0.13

≤0.35

≤0.70

≤0,025

≤0,020

≤0.30

≤0.06

≤0.30

≤0.30

/

P235

≤0.16

≤0.35

≤1.20

≤0,025

≤0,020

≤0.30

≤0.06

≤0.30

≤0.30

/

P265

≤0.20

≤0.40

≤1.40

≤0,025

≤0,020

≤0.30

≤0.06

≤0.30

≤0.30

/

EN10216-2

P195GH

≤0.13

≤0.35

≤0.70

≤0,025

≤0,020

≤0.30

≤0.06

≤0.30

≤0.30

/

P235GH

≤0.16

≤0.35

≤1.20

≤0,025

≤0,020

≤0.30

≤0.06

≤0.30

≤0.30

/

P265GH

≤0.20

≤0.40

≤1.40

≤0,025

≤0,020

≤0.30

≤0.06

≤0.30

≤0.30

/

13CrMo4-5

0.100.17

≤0.35

0.400.70

≤0,025

≤0,020

0.701.15

0.400.60

≤0.30

≤0.30

/

10CrMo9-10

0.080.14

≤0,50

0.300.70

≤0,025

≤0,020

2.002.50

0.901.10

≤0.30

≤0.30

/